Nov 9 - 30: Free Lightburn Pro with every laser > $2,000* | 75-day Extended Returns
Nov 9-30: Free Lightburn Pro with every laser > $2,000*
Skip to content
THEO MA1-35 handheld laser welder for troubleshooting common laser weld defects

Handheld Laser Welding Defects: Porosity, Burn-Through, Undercut and Cracking (Causes and Fixes)

Short answer: most handheld laser welding defects come from four places, in this order: dirty metal, shielding gas problems, poor fit-up and settings. New operators often start by changing power, but power is rarely the first thing to fix. Porosity is almost always contamination or gas. Burn-through and undercut are usually too much heat for the gap and thickness. Cracking is mostly a material problem (alloy, filler or cooling rate). This guide covers each defect, how to recognize it and what to change, with a troubleshooting table at the end you can print for the shop.

Based on the calls our team fields every week from laser welder owners, these are the defects people ask us about, and most can be fixed with prep, gas and settings rather than new equipment.

Table of Contents

Troubleshoot in the Right Order

Change one variable at a time, and work from cheapest and most likely to least likely:

  1. Clean the joint. Oil, paint, mill scale, oxide and moisture cause most porosity and spatter.
  2. Check the gas. Right gas, right flow, no leaks, nozzle not clogged.
  3. Check fit-up. Gap, alignment and clamping. Our fit-up and gap tolerance guide explains why this matters more than wattage.
  4. Check the optics. A dirty or pitted protective lens absorbs power and shifts results.
  5. Then adjust settings: travel speed, power, wobble width and frequency, wire feed speed.

Porosity

What it looks like: pinholes on the bead surface, or voids you only find when you cut or bend a coupon.

Common causes

  • Contamination: oil, coolant, paint, galvanizing, oxide layers (especially on aluminum) and moisture.
  • Gas problems: too little flow, too much flow (turbulence pulls in air), a leak in the line, drafts from fans or open doors, or the wrong gas for the metal.
  • Unstable keyhole: deep, narrow welds can trap gas when the keyhole collapses, particularly at the end of a weld.
  • Zinc or other volatile elements: galvanized steel and brass release vapor that bubbles through the pool.

Fixes

  • Degrease with acetone and remove oxide just before welding. On aluminum, clean within a few hours of welding; the oxide reforms.
  • Leak-check fittings, confirm the flow at the nozzle and shield the area from drafts. See our shielding gas guide.
  • Use a moderate wobble to keep the pool open longer so gas can escape.
  • Ramp down at the end of the weld rather than stopping abruptly.

If porosity appears on a new machine, fix cleanliness and gas coverage before touching the factory settings. Those two account for far more porosity than the laser itself.

Burn-Through

What it looks like: holes through thin sheet, or a sagging bead on the back side.

Common causes

  • Too much power or too slow travel for the thickness.
  • A gap the beam falls straight through, especially on 16-gauge (about 1.5 mm) and thinner sheet.
  • Heat building up on a long weld or a small part.

Fixes

  • Increase travel speed before you lower power. Laser welders are designed to move fast.
  • Close the gap, or add filler wire to bridge it (see fusion vs wire-fed laser welding).
  • Use a wider wobble to spread heat on thin material.
  • Stitch weld or skip around the part to manage heat; use a copper or aluminum backing bar.
  • Start from the thin-sheet preset on your machine rather than a generic one.

Undercut and Concave Beads

What it looks like: a groove melted into the base metal along the edge of the weld, or a bead that sits below the surface.

  • Causes: too much heat for the joint, travel too fast for the amount of metal being melted, a gap with no filler, or the beam aimed off the joint line.
  • Fixes: add filler wire to supply metal, reduce power slightly, slow down a little, and re-aim the torch so the beam is centered. On fillet welds, adjust the torch angle so both faces are melting evenly.

Undercut is a stress concentrator, so it matters on structural parts even if the weld looks clean.

Cracking

What it looks like: a line down the center of the bead (centerline crack), small cracks at the end crater, or cracks in the heat-affected zone.

Common causes

  • Crack-sensitive alloys: some aluminum alloys (for example 6061 welded without filler), high-carbon and some tool steels, and certain dissimilar-metal combinations.
  • Fast cooling: laser welds cool very fast, which raises hardness in hardenable steels.
  • Crater cracks from stopping abruptly.
  • Restraint: clamping that doesn't let the part move as it shrinks.

Fixes

  • Use the right filler: ER4043 or ER5356 on 6xxx-series aluminum changes the weld chemistry and greatly reduces cracking.
  • Preheat hardenable steels where the procedure calls for it.
  • Use a ramp-down or fill the crater at the end of the weld.
  • Reduce restraint or sequence welds to balance shrinkage.

For aluminum specifics, read why aluminum is tricky to laser weld.

Lack of Fusion and Shallow Penetration

What it looks like: a weld that looks fine on top but breaks along the joint line in a bend test, or no visible penetration on the back side.

  • Causes: too little power or too much speed for the thickness, beam missing the joint line, focus or stand-off off, a dirty protective lens, or highly reflective metal (copper, polished aluminum).
  • Fixes: slow down or add power, keep the nozzle in correct contact, check and replace the protective lens, and verify that the beam lands on the seam. If the part is near your machine's rated depth, it may simply be beyond what your power level can do reliably; see how much power your laser welder needs.

You can't see lack of fusion from the top. Prove it with coupons: our guide to verifying laser weld penetration covers bend tests, macro-etch and NDT.

Spatter, Humping and Rough Beads

  • Spatter: usually contamination, galvanizing or an unstable keyhole from excessive power. Clean the part, reduce power slightly and check gas flow.
  • Humping (a beaded, uneven ridge): travel speed too high for the power. Slow down or widen the wobble.
  • Irregular bead width: inconsistent hand speed or torch angle. Brace your hand, use a guide where possible, and practice on straight seams.
  • Wire stubbing or balling: wire speed too fast (stubbing) or too slow (balling), or the wire is not entering the beam spot.

Discoloration and Oxidation

Straw to blue tint on stainless is a sign of heat and oxygen exposure. Gray or black, sooty beads mean poor shielding.

  • Improve gas coverage and check for drafts.
  • Shield the back side on stainless where corrosion resistance matters (food and pharma work).
  • Increase travel speed to reduce heat input.
  • Clean up tint with a laser cleaner, pickling paste or an electrolytic weld cleaner. Many machines include a cleaning mode for this.

Quick Troubleshooting Table

Defect Check first Then adjust
Porosity Cleanliness, gas leaks and flow, drafts Add wobble, ramp down at the end
Burn-through Gap, thickness vs preset Faster travel, then less power; add wire
Undercut Beam aim, gap Add wire, slightly less power
Cracking Alloy and filler choice Correct filler, ramp-down, preheat where needed
Lack of fusion Protective lens, beam on seam Slower travel or more power
Spatter Contamination, coatings Slightly less power
Discoloration Gas coverage, back shielding Faster travel

When It's the Machine, Not the Setup

Suspect setup if the defect appears on some parts but not others, changes when you clean the metal or adjust gas, or started after a lens or nozzle change.

Suspect the machine if output drops on clean, well-fitted coupons that welded fine last week, the machine throws faults, or results change with no change in setup. Then log the error codes and settings and contact the dealer or manufacturer.

Suspect the machine is undersized if you're consistently welding near its rated depth and see shallow fusion or need very slow speeds. That's a sizing problem, not a defect. Based on our experience selling laser welders to universities, schools and fabrication shops of all sizes, we recommend buying with headroom above your thickest regular job to avoid it.

Frequently Asked Questions

Why are my laser welds porous?

Usually contamination (oil, oxide, coatings) or shielding gas problems (leaks, wrong flow, drafts). Clean the joint and check the gas line before changing power.

How do I stop burning through thin sheet with a laser welder?

Speed up first, then reduce power, close the gap or add filler wire, and use a wider wobble. A backing bar helps on very thin material.

Why does my aluminum laser weld crack?

Many aluminum alloys, especially 6061, are crack-sensitive when welded without filler. Use ER4043 or ER5356 wire and ramp down at the end of the weld.

How can I tell if a laser weld has full penetration?

Look for consistent fusion on the back side, then confirm with a bend test or a cut-and-etch cross-section on a test coupon.

What causes undercut in laser welding?

Too much heat for the joint, a gap without filler or the beam aimed off the seam. Add filler, reduce power slightly and re-center the torch.

Is spatter normal with a handheld laser welder?

Some spatter on coated or dirty metal is normal, but clean steel should weld with very little. Heavy spatter usually means contamination or too much power.

Chasing a weld defect you can't fix? Contact The Maker's Chest with a photo of the weld, your material and settings, and our team will help you track it down.

Written By

Alina Oprea profile picture

Alina Oprea

Maker & Equipment Specialist

Alina Oprea is a hands-on maker, jeweler, and workshop specialist at The Maker’s Chest, with 25 years of silversmithing experience alongside a background in woodworking, renovations, construction, and commercial ductwork installation.

Her experience spans decorative woodwork, hand-carved doors, jewelry fabrication, homebuilding with Habitat, and real jobsite problem-solving — giving her a practical understanding of materials, tools, workflow, and what machines need to deliver beyond the spec sheet.

Next article Laser Welding Copper and Brass: Why Reflectivity and Beam Quality Matter
Skip the AI. Call an Expert. Skip the AI. Call an Expert.